A Study of the Possibility of Obtaining Prolonged-release Solid Dispersions of a Water-soluble Drug

 

Ranim Alrouhayyah1,2, Svetlana N. Suslina1

1Department of General Pharmaceutical and Biomedical Technology, Institute of Medicine,

RUDN University, 6 Miklukho-Maklaya St, Moscow, 117198, Russian Federation.

2Department of Analytical and Food Chemistry, Faculty of Pharmacy, Damascus University, Damascus, Syria.

*Corresponding Author E-mail: alrukhaie-r@rudn.ru

 

ABSTRACT:

The aim of this study was to evaluate the feasibility of obtaining prolonged-release solid dispersions of trimetazidine dihydrochloride using kollidon® SR and PolyoxTM WSR 303 in various ratios as drug release-slowing polymers. Solid dispersions in the ratios of 1:2, 1:4 and 1:8 (drug: polymer) were prepared by solvent evaporation method using isopropanol as solvent. The prepared formulations were evaluated for drug content uniformity, flowability, compressibility, weight loss on drying, and dissolution profile. Structural and morphological characteristics were assessed using X-ray diffraction and microscopy. Uniform distribution of the drug throughout the polymer matrix was demonstrated for all formulations, with drug content varying from 97.14 to 103.33%. The weight loss on drying was in the range of 1.12-2.84%, and flowability and compressibility were within the satisfactory range, varying from fair to excellent. Increasing the proportion of polymer reduced the dissolution rate, enabling prolongation of the drug release up to 12 h with Kollidon® SR. However, a prolonged-release profile could not be obtained in solid dispersions prepared with PolyoxTM WSR 303. X-ray diffraction confirmed the formation of solid dispersions and the absence of polymorphism, while microscopy provided morphological evidence of solid dispersion formation. The results of this study demonstrate that prolonged-release solid dispersions of the water-soluble drug trimetazidine dihydrochloride can be obtained by solvent evaporation method using appropriate polymers in suitable ratios.

 

KEYWORDS: Trimetazidine dihydrochloride, Water-soluble drug, Solid dispersion, Kollidon® SR, PolyoxTM WSR 303, Prolonged release.

 

 


INTRODUCTION: 

Modified-release, including prolonged-release, dosage forms are intended to minimize problems associated with traditional dosage forms, such as fluctuations in plasma drug concentrations and the need for frequent dosing1,2, thereby improving patient adherence to treatment and/or drug efficacy3,4.

 

Although solid dispersion technology is most often associated with solving the problem of poor solubility5’6, it has recently been increasingly used to develop prolonged-release systems not only for poorly soluble but also for soluble drugs7. These systems combine the advantages of both solid dispersions and prolonged-release systems, while largely eliminating the risk of sudden drug release8’9.

 

Trimetazidine dihydrochloride (TMD), [1-(2,3,4-trimethoxybenzyl)-piperazine dihydrochloride], is an antianginal drug with no negative inotropic or vascular properties10 that improves myocardial glucose utilization by selectively inhibiting fatty acid oxidation11.

 

TMD is freely soluble in water, with a plasma half-life of about 6.0±1.4 h and Tmax of 1.80±0.7 h12, making the development of prolonged-release formulations particularly relevant given its favorable safety profile and long-term use in the management of chronic ischemic conditions. However, the development of prolonged-release formulations is complicated by its high water solubility.

 

Considering the pharmacological and biopharmaceutical characteristics of TMD, it is advisable to develop prolonged-release dosage forms that not only maintain its therapeutic efficacy but also improve its technological and biopharmaceutical properties. Therefore, the development of solid dispersions of TMD is proposed as a novel approach to producing prolonged-release systems for highly water-soluble drugs.

 

In this work, we aimed to evaluate the feasibility of formulating prolonged-release solid dispersions of TMD using Kollidon® SR and Polyox™ WSR 303 at different drug:polymer ratios.

 

Kollidon® SR is a white or slightly yellowish free-flowing powder which is a physical mixture of 80% polyvinyl acetate (a plastic material that produces a coherent matrix when compressed) and 19% povidone (a soluble pore-forming material), with approximately 0.8% sodium lauryl sulfate and 0.2% silicon dioxide as stabilizers13. It can be used to get prolonged-release solid dosage forms by various technologies such as direct compression, wet granulation and extrusion, in different ratios depending on the solubility of the active pharmaceutical ingredients14’15.

 

Polyox™ is a group of nonionic polymers of poly(ethylene oxide). They are white to off-white, free-flowing, hydrophilic powders available in a wide range of viscosity grades corresponding to molecular weights ranging from approximately 100,000 to 7,000,000 Da. Polyox™ polymers exhibit thermoplastic properties, rapidly hydrate, and quickly form hydrogels15’16. Among various Polyox™ grades, Polyox™ WSR 303 is widely used as a binder in controlled-release matrix tablets owing to its rapid hydrogel-forming ability and lubricity. It has a high molecular weight of approximately 7,000,000 Da and a viscosity in the range of 7,500-10,000 mPa.s17.

 

MATERIAL AND METHODS:

Material:

Trimetazidine dihydrochloride (CAS 5011-34-7, Alcon biosciences private limited, India), Kollidon® SR (CAS 264876-68-8, BASF, Germany), PolyoxTM WSR 303 (CAS 25322-68-3, DuPont, USA), isopropanol (CAS 67-63-0, Chimmed, Russia). All other chemicals were of analytical grade.

Preparation of solid dispersions:

Solid dispersions (SDs) were prepared with each polymer in three TMD:polymer ratios of 1:2, 1:4, and 1:8 (Table 2) by solvent evaporation method, where TMD was dissolved in excess amount of isopropanol, followed by the addition of the polymer with continuous stirring until a homogeneous solution was obtained. The isopropanol was then removed under vacuum using a rotary evaporator (Heidolph Laborota 4002 control HB/G1, Germany) at a temperature of 50±2 °C until a thin film was formed. The resulting film was crushed in a mortar and passed through a sieve with a 1 mm mesh size.

 

The obtained formulations were subjected to the following tests, which were primarily conducted in accordance with the requirements of the State Pharmacopoeia of the Russian Federation, 15th edition18:

 

Content uniformity:

To assess the uniform distribution of TMD in the polymer matrix, the drug content was determined in 5 precisely weighed portions (10 mg TMD) of each formulation. Each portion was ground in a mortar in an appropriate amount of 0.1M HCl. The resulting suspension or solution (based on the solubility of the polymer in 0.1M HCl) was placed in a 50 ml measuring flask (considering washing the mortar and pestle with the used solvent), brought to the mark with 0.1 M HCl and filtered. The optical density of the filtrate was measured on spectrophotometer (СФ-103 single-beam scanning spectrophotometer, Russia) at λmax= 269 nm, after appropriate dilution, and the concentration was determined using a pre-plotted calibration curve19. The amount of TMD in each portion was determined, and the drug content (%) was expressed as mean ± standard deviation.

 

Pharmaceutical-technological characteristics:

Since SDs are intended for use in the manufacture of various dosage forms, including tablets and capsules, the following pharmaceutical-technological properties were evaluated:

 

Flowability and compressibility:

a.     Angle of repose: SD flowed out of the funnel opening onto a flat horizontal surface, and the height and diameter of the formed cone were measured to determine the tangent of the angle of repose, which was then calculated in degrees.

b.     Density tests: they were performed using a tapped density tester (Erweka GmbH SVM II, Germany), to determine bulk density (DB) and tapped density (DT). Hausner ratio and Carr’s index (compressibility coefficient) were subsequently calculated as follows:

Hausner ratio = DT/ DB,

Carr’s index = [(DT- DB)/ DT] × 100%

The tests of flowability and compressibility were repeated 3 times for each formulation, and the results were expressed as mean ± standard deviation.

 

Weight loss on drying:

Measurements were conducted at a temperature of 105±2 ºC on 3 samples (1-2 g each) of each formulation, using an infrared moisture analyzer (Aquilon AV-50, Russia). Results are presented as mean ± standard deviation.

 

Dissolution test:

The test was conducted on 6 samples (each containing 50 mg TMD) of each formulation using a dissolution apparatus (Raytor RT 600, China); paddle type, 50 r/min in 900 ml of hydrochloric acid (0.1 M) for the first two hours, then 900 ml of phosphate buffer (pH = 6.8) for the remaining time, and t=37±0.5 °C all over the time of the experiment. Samples of 5 ml were withdrawn at certain intervals and replaced with 5 ml of pure medium (acid or buffer). The withdrawn samples were filtered (through filters fixed on the sampling needles of the apparatus). The absorbance of the filtrates was measured at λmax= 269 nm, and the release of TMD was quantified using a pre-plotted calibration curve (in acidic medium or in phosphate buffer)19. 

 

Release kinetics:

The kinetics of TMD release from the obtained prolonged-release SDs were evaluated by fitting the in vitro dissolution data to several kinetic models (Table 1). The correlation coefficient (r2) and rate constant were determined for each model.


 

Table 1: The considered kinetic models of drug release20,21

Kinetic model

Equation

Symbol interpretation

Zero order

Mt = Ko t

Mt- the amount of drug released over time t,

M0- the initial amount of the drug,

M- the amount of drug remaining at time t,

M∞- the amount of drug released at infinite time,

K0, K1, KH, KHC, KRP: rate constants for zero order, first order, model Higuchi, model Hixson-Crowell, model Ritger –Peppas, respectively.

n: the degree of release associated with the release mechanism, where:

n≤0.45: diffusion according to Fick's law;

0.45<n<0.89: anomalous diffusion, i.e. drug release is controlled by diffusion and erosion;

n>0.89: case II transport, i.e. transport of the drug molecules within the polymer is a result of degradation of the polymer matrix.

First order

Log (M0/M)  = K1 t/2.303

Model Higuchi

Mt = KH t1/2

Model Hixson-Crowell

M01/3 – M1/3 = KHC t

Model Ritger -Peppas

Mt /M∞ = KRP tn

 


X-ray diffraction (XRD):

The analysis was performed using a diffractometer (D8 Advance, Germany) with Cu Kα radiation. The X-ray tube was operated at a voltage of 40 kV and a current of 30 mA. The x-axis of the XRD pattern shows the doubled diffraction angle (2θ) in degrees, and the y-axis shows the intensity in counts. Measurements were carried out in the 2θ range from 5° to 70° with a step of 0.05° and with an exposure at a point of 1 s, the sample was rotated.

 

Microscopy:

The study was performed for TMD and polymers as pure materials, as well as for SDs, using a digital microscope (Saikedigital, China.). A small amount (about 10-20 mg) of the powder being studied was placed on a glass slide, mixed with vaseline oil (1-2 drops), covered with a cover glass and examined under the microscope.

 

RESULTS AND DISCUSSION:

SDs in ratios of 1:2, 1:4 and 1:8 (TMD:polymer) were prepared by solvent evaporation method using isopropanol as solvent and Polyox™ WSR 303 and kollidon® SR as polymer capable of prolonging drug release. The choice of "solvent evaporation" method is due to the fact that the solvent promotes disintegration and homogenization of components at the molecular level, ensuring complete and close interaction of the SD ingredients. Also, after the solvent is removed, the carrier maintains the molecularly dispersed state of the active pharmaceutical ingredient (API), preventing or slowing down recrystallization during storage. Furthermore, this method does not require significant heating, which helps to avoid thermal decomposition of the polymer and the API22.

 

API TMD was evenly distributed in SDs and its content in all prepared formulations ranged from 97.14 to 103.33% (Table 2). The obtained SDs showed satisfactory technological characteristics: the weight loss on drying was in the range of 1.12-2.84%; flowability and compressibility, assessed by the values of the angle of repose, Carr’s index and Hausner ratio, ranged from fair to excellent (Table 2). These results indicate the suitability of the prepared formulations for further pharmaceutical processing, such as direct compression tabletting.


 

Table 2: Formulation and characteristics of prepared solid dispersions

Formulation

Characteristics

Drug content, %

Angle of repose, º

Hausner ratio

Carr’s index, %

Weight loss on drying, %

Dissolution time, h

SDk1 (TMD:Kollidon® SR- 1:2)

101.24±2.09

28.5±0.02

1.08±0.006

7.78±0.23

2.18±0.02

2

SDk2 (TMD:Kollidon® SR- 1:4)

98.84 ±0.77

27.9±0.01

1.09±0.006

8.45±0.22

2.81±0.03

9

SDk3 (TMD:Kollidon® SR- 1:8)

101.10± 0,84

26.9±0.02

1.09±0.006

8.09±0.33

2.68±0.03

13

SDp1 (TMD:Polyox™ WSR 303-1:2)

98.96 ±0.95

29.44±0.01

1.19±0.006

15.88±0.50

1.97±0.02

0,1

SDp2 (TMD:Polyox™ WSR 303- 1:4)

100.05 ±2.68

33.21±0.03

1.17±0.010

14.78±0.30

1.13±0.01

0,5

SDp3 (TMD:Polyox™ WSR 303-1:8)

99.99±2.85

31.16±0.05

1.16±0.006

13.68±0.45

2.17±0.02

1

 


The dissolution time of prepared SDs varied depending on the type and the proportion of the polymer, with an inverse correlation being observed between the polymer proportion and the dissolution rate for both polymers: as the polymer content increased, the dissolution rate of TMD decreased. However, Polyox™ WSR 303 failed to prolong the drug release in the formulations studied (SDp1, SDp2, SDp3), although, according to the literature, this polymer is successfully used to prepare prolonged-release tablets. This may be explained by the fact that the dissolution of TMD from SDs occurs faster than the swelling of the polymer and, consequently, the formation of a gel barrier capable of slowing the drug release. This gel barrier is the key mechanism underlying drug release from prolonged-release tablets based on PolyoxTM. Also, 70% of the TMD contained in SDk1 (TMD: Kollidon® SR 1:2) was dissolved within 2 hours, but increasing the proportion of Kollidon® SR resulted in delayed TMD release up to 9 hours in SDk2 and 13 hours in SDk3, which is consistent with the objective of our study to obtain prolonged-release SDs of TMD.

 

Several kinetic models were used to mathematically describe the mechanism of TMD release and characterize the dissolution kinetics of SDk2 and SDk3 (in which prolonged release of TMD was observed). The calculated parameters for each model are presented in Table 3. It turned out that not only one model showed good linearity, indicating a combination of multiple drug release mechanisms rather than a single mechanism. However, the best fit with a higher correlation was found using the Higuchi model and the Hixson-Crowell model. This suggests that TMD release from SDs occurs via diffusion through pathways formed within the matrix, with release being controlled by the diffusion barrier of the gel and/or surface erosion. Furthermore, the Ritger-Peppas model showed good linearity with “n” values in the range of 0.45-0.89, indicating a combined release mechanism involving both API diffusion and polymer degradation/erosion (Table 3).

 

XRD analysis demonstrated the crystalline nature of pure TMD, evidenced by the presence of characteristic diffraction peaks (Fig. 1a). In the diffraction patterns of SDs (Fig. 1), these peaks were absent or their intensity was significantly reduced, indicating a substantial loss of crystallinity. Furthermore, comparison of the XRD patterns of pure TMD (Fig. 1a).and TMD recrystallized in isopropanol (Fig. 1b).revealed no peak shift or significant changes in intensity, indicating the absence of polymorphism.

 

The microscopic findings corroborated the XRD data, confirming the crystalline nature of TMD and revealing the structural changes induced by the formation of SDs. The resulting SDs were characterized by non-spherical, irregularly shaped particles (Fig. 2).


 

Table 3: Calculated parameters of kinetic models applied to SDk2 and SDk3 formulations

Formulation

Kinetic model

Zero order

First order

Higuchi

Hixson- Crowell

Ritger -Peppas

r2

K

r2

K

r2

K

r2

K

r2

n

K

SDk2

0.9646

13.55

0.9290

0.194

0.9979

33.94

0.9953

0.405

0.9976

0.56

30.80

SDk3

0.9353

9.87

0.9838

0.146

0.9874

30.28

0.9974

0.307

0.9865

0.55

27.84

 

 

 

(a) TMD

(b) TMD recrystallized in isopropanol



 

(c) Kollidon® SR

 

(d) PolyoxTM WSR 303

 

(e) SDk2

 

(f) SDp2

 

(g) SDk3

 

(h) SDp3

Figure 1: XRD patterns of TMD, Kollidon® SR, PolyoxTM WSR 303, and corresponding SDs

 

 

 

 


 

Figure 2: Microphotographs (10× magnification) of TMD, Kollidon® SR, PolyoxTM WSR 303, and corresponding SDs

 


CONCLUSION:

Solid dispersions of trimetazidine dihydrochloride (TMD) were prepared by solvent evaporation method using Kollidon® SR and PolyoxTM WSR 303 as carrier and isopropanol as solvent. Structural characterization confirmed the formation of solid dispersions with no detectable polymorphic forms. The obtained formulations exhibited satisfactory pharmaceutical-technological characteristics, suitable for further pharmaceutical processing. Dissolution testing revealed that Polyox™ WSR 303 did not provide a prolonged-release profile in the investigated ratios. Similarly, the Kollidon® SR formulation at 1:2 (TMD:polymer) ratio did not achieve the desired prolonged release. In contrast, increasing the TMD: Kollidon® SR ratio to 1:4 and 1:8 resulted in prolonged-release solid dispersions, with TMD release extending up to 9 and 13 hours, respectively. The dissolution kinetics for obtained prolonged-release solid dispersions were well described by Higuchi and Hixson-Crowell models, while the Ritger-Peppas model indicated anomalous diffusion as the main release mechanism. The findings of this study demonstrate that solid dispersion technology, combined with the strategic selection of appropriate carriers and optimized drug:polymer ratios, is a promising approach for prolonging the release of water-soluble drugs.

 

ACKNOWLEDGMENT:

Authors are thankful to Mirpharm Pharmaceutical Company (Russia) for providing TMD and polymers.

 

CONFLICT OF INTEREST:

The authors have no conflicts of interest.

 

REFERENCES:

1.      Vilas A, Siddheshwar SS. A Review on Floating Microsphere. Asian J. Pharm. Tech. 2024; 14(1): 31-35. doi: 10.52711/2231-5713.2024.00007.

2.      Madat DV, Gohel MC, Ramkishan A. Development of Venlafaxine Hydrochloride Controlled Release Pellets Prepared Employing the Blend of Ethyl Cellulose and Polyethylene Oxide. Research J. Pharm. and Tech. 2012; 5(10): 1289-1292.

3.      Rahul Kh, Nilkanth B, Nilesh K. A Review on Applications of Hydroxy Propyl Methyl Cellulose and Natural polymers for the development of modified release drug delivery systems. Research J. Pharm. and Tech. 2021; 14(2): 1163-1170. doi: 10.5958/0974-360X.2021.00208.0.

4.      Parikshit P. A Review on Nanoparticle-Loaded Hydrogels for Extended Drug Release. Asian J. Pharm. Tech. 2024; 14(1): 55-58. doi: 10.52711/2231-5713.2024.00011.

5.      Pradeep NSh. A Review: Increasing Solubility of Poorly Soluble Drugs by Solid Dispersion Technique. Research J. Pharm. and Tech. 2011; 4(12): 1933-1940.

6.      Alrouhayyah R, Sheshko TF, Suslina SN [et al]. Solid Dispersions: An Effective Technology for Improving Dissolution Kinetics of Poorly Soluble Drugs. Research J. Pharm. and Tech. 2023; 16(12): 5701-6. doi: 10.52711/0974-360X.2023.00922

7.      Alrouhayyah R, Suslina SN. Solid Dispersions: Improved Solubility and Sustained Release. Am J Biomed Sci & Res. 2024; 21(6). AJBSR.MS.ID.002903, DOI: 10.34297/AJBSR.2024.21.002903.

8.      Patel K, Shah Sh, Patel J. Solid dispersion technology as a formulation strategy for the fabrication of modified release dosage forms: A comprehensive review. Daru 2022; 30(1): 165-189.

9.      Bhosale N, Velhal A, Redasani VK [et al]. An overview on sustained release formulations using solid dispersion as solubility enhancement technique. Asian Journal of Pharmaceutical Research and Development. 2023; 11(3): 84-91. DOI: http://dx.doi.org/10.22270/ajprd.v11i3.1257.

10.   Barokar AA, Wagh RD, Baviskar DT [et al.]. Formulation and Characterization of Taste Masked Rapid Disintegrating Tablets of Trimetazidine HCl. Research J. Pharm. and Tech. 2011; 4(7): 1098-1102.

11.   Hemant KJ, Deepak DD. Development and Validation of Spectrophotometric Method for Determination of Trimetazidine Hydrochloride in Bulk and Tablet Dosage Form. Research J. Pharm. and Tech. 2016; 9(9): 1457-1460. doi: 10.5958/0974-360X.2016.00282.1.

12.   Dandagi PM, Singh A, Manvi FV [et al]. Formulation and effect of viscosity and concentration of methocel on release characteristics of trimetazidine matrix tablets. International Journal of Pharmacy and Pharmaceutical Sciences. 2012; 4(1): 230-235.

13.   Fouad EA, Ibrahim MA, El-Badry M. Embedment of Chlorpheniramine Maleate in Directly Compressed Matrix Tablets of Compritol and Kollidone SR. Trop J Pharm Res. 2015; 14(3): 371-377.

14.   Sakr W, Alanazi F, Sakr A. Effect of Kollidon® SR on the release of Albuterol Sulphate from matrix tablets. Saudi Pharmaceutical Journal. 2011; 19(1): 19-27. https://doi.org/10.1016/j.jsps.2010.11.002.

15.   Sheskey PJ, Cook WG, Gable CG. Handbook of Pharmaceutical Excipients, 8th ed. Pharmaceutical Press: London, UK and American Pharmacists Association: Washington, USA. 2017; 1184p.

16.   Kotsur J, Flisyuk EV. Modern polymers in prolonged release tablet technology. Pharmacy Formulas. 2020; 2(1): 36-43. DOI:10.17816/phf21267. (in Russian)

17.   Shah AP, Bhandary SR. POLYOX (polyethylene oxide) - applications in pharma industry. Pharmaceutical Reviews. 2010; 8(3).

18.   State Pharmacopoeia of the Russian Federation. 15th ed. (2023). Moscow. URL: https://phar-macopoeia.regmed.ru/pharmacopoeia/izdanie-15/?ysclid=me2g4hcj30860500137 (accessed 31.07.2025). (In Russ.).

19.   Alrouhayyah R, Suslina SN. Development and validation of an accessible analytical method for the quantification of trimetazidine dihydrochloride for research purposes. Journal of Siberian Medical Sciences. 2024; 1: 64-74. (In Russ.) https://doi.org/10.31549/2542-1174-2024-8-1-64-74.

20.   Patel AJ, Singh RP, Patel V [et al]. Application of Mathematical Models in Drug Release Kinetics of Lagerstroemia Speciosa Extract-Phospholipid Complex. Research J. Pharm. and Tech. 2022; 15(3): 1257-1262. doi: 10.52711/0974-360X.2022.00210.   

21.   Alrouhayyah R, Dahma N, Bratchikova IG. A Study of the effect of some Formulation and Preparation variables on Drug Release from Matrix Tablets. Research J. Pharm. and Tech. 2025; 18(1): 345-354. doi: 10.52711/0974-360X.2025.00054.

22.   Malkawi R, Malkawi WI, Al-Mahmoud Y [et al]. Current Trends on Solid Dispersions: Past, Present, and Future. Advances in Pharmacological and Pharmaceutical Sciences. 2022; 17p. https://doi.org/10.1155/2022/5916013.

 

 

 

 

Received on 16.08.2025      Revised on 08.10.2025

Accepted on 07.12.2025      Published on 08.08.2026

Available online from August 12, 2026

Research J. Pharmacy and Technology. 2026;19(8):3721-3726.

DOI: 10.52711/0974-360X.2026.00525

© RJPT All right reserved

 